How Malleable Iron Pipe Fittings Are Made: 16 Stages from Pattern to Container

PT Tri Sinar Purnama · 21 November 2026 · 3 min read

Baca dalam Bahasa Indonesia →

Malleable iron pipe fittings are made by foundry casting: iron is melted, poured into sand moulds, annealed to become ductile, then cleaned, galvanized if required, threaded, tested and packed. At PT Tri Sinar Purnama the whole sequence runs in-house in 16 stages.

Quick Answer

Key stages:

  • Patterns & cores → sand moulding → cupola melting → casting.
  • Annealing makes the cast iron ductile.
  • Hot-dip galvanizing happens before threads are cut.
  • Threads are gauge-checked; 100% of products are leak-tested before packing.

TSP’s 16 production stages

#StageWhat happens
01Pattern makingTooling and patterns defining each fitting’s geometry are made in-house
02Pattern preparationPatterns are mounted, checked and set up for moulding
03Core makingSand cores for internal bores and cavities are produced and cured
04Moulding sand preparationSand is mixed and conditioned; compactibility tested every 30 minutes
05MouldingMoulds are formed on jolt squeeze lines and assembled with cores
06Melting & castingIron is melted in cupola furnaces and poured; chemistry checked by spectrometer
07AnnealingCastings are heat-treated to become ductile
08GrindingGates, risers and parting lines are removed
09Shot blastingCastings are cleaned before coating and machining
10GalvanizingHot-dip galvanizing; coating thickness checked with an Elcometer
11TappingThreads cut to standard and checked with plug & ring gauges
12Lathe / machiningTurning and machining, including unions
13DryingProducts are dried before final inspection
14Packing100% leak testing before packing
15Finished goods warehouseStock is held and staged for despatch
16Container loadingExport orders are loaded for shipment

Source: trisip.com Manufacturing page.

Quality checkpoints along the route

StageCheckCriterion / frequency
Moulding sandCompactibility testEvery 30 minutes
MeltingSpectrometer chemistry4 times a day
After castingTensile & elongationMin. 350 N/mm², elongation min. 6%
GalvanizingZinc thickness (Elcometer)10 spots per sample, min. 70 µm
TappingPlug & ring gauges3 pcs per machine every 30 minutes
Before packingLeak test100% of products, min. 7 bar > 3 s
Before shipmentAQL inspectionSampling before shipment

Source: trisip.com Quality Control page.

Why in-house production matters to buyers

When every stage is done by one manufacturer, each fitting can be traced from melting to packing and quality procedures stay consistent. TSP runs this route across two production sites totalling 60,000 m², with 15,600 tons of annual capacity and more than 1,900 employees (About).

Conclusion

A malleable iron fitting comes out of a long foundry route: pattern, mould, melting, annealing, galvanizing, threading, testing and packing. At TSP these 16 stages are done in-house, with measurable quality checkpoints at each key step.

Fittings from an integrated foundry

PT Tri Sinar Purnama has made malleable iron fittings in-house in Semarang since 1983.

Frequently Asked Questions

How are malleable iron fittings made?

Iron is melted in cupola furnaces, poured into sand moulds, annealed, ground and cleaned, galvanized if required, threaded, leak-tested and packed.

What does annealing do?

Annealing is a heat treatment that changes the carbon structure of the cast iron so the material becomes ductile instead of brittle.

Are threads cut before or after galvanizing?

At TSP, threads are tapped after galvanizing (stage 11, after stage 10).

What is TSP’s production capacity?

15,600 tons per year across two production sites totalling 60,000 m².

How does TSP make sure fittings do not leak?

100% of products are leak-tested at a minimum of 7 bar held for more than 3 seconds before packing.